Polar Ice Casting Slip is our cone 6 porcelain made as a casting body and sold as a dry powder, so you mix the slip yourself with water and Darvan No. 7. The recipe below aims for a specific gravity of about 1.7 and a Ford Cup viscosity of 40 seconds. It is a reliable starting point, but the Darvan and water amounts may need small adjustments for your materials, so keep notes as you go.
Start with the small test batch. Do not mix a full 20 kg bag first. Too much Darvan (over-deflocculation) can turn the whole bucket into an unusable jelly that has to be thrown out.
The recipe
| Ingredient | % by weight | Test batch | 1 US gallon | Full 20 kg bag |
| Polar Ice Casting Slip powder | 67.3 | 673 g | 5,000 g | 20 kg |
| Water (distilled recommended) | 32 | 320 g | 2,377 g | 9.5 kg |
| Darvan No. 7 | 0.7 | 7 g | 52 g | 208 g |
As a guide to yield, 5,000 g of powder makes about 1 US gallon of slip, and 6,300 g makes about 1 Canadian gallon.
Mixing steps
- Weigh everything for the batch size you chose.
- Add 90% of the Darvan to the water and stir it in. That is about 6.3 g for the test batch, 47 g for the 1 US gallon batch and 187 g for a full bag. Keep the other 10% aside.
- Add the powder slowly to the water while running a propeller mixer.
- Mix for at least 15 minutes.
- If the last of the powder will not go in, add the Darvan you kept aside and keep mixing.
Check and adjust
Specific gravity
- Too high: add water. In a 1 US gallon batch, 50 g of water lowers the specific gravity by about 0.01, for example from 1.79 to 1.78.
- Too low: leave this batch as it is, and make a note to use less water next time.
New to measuring specific gravity? The simple 100 ml method in our M370 Casting Slip Preparation article works the same way for Polar Ice.
Viscosity
- Not fluid enough: mix longer, ideally another 30 minutes, or let the slip sit overnight and power mix it the next day.
- Still too thick: add a small amount of water. Keep in mind this also lowers the specific gravity.
Your first casts
If the inside surface looks powdery or dry shortly after you pour out the slip, there is too much Darvan in the slip.
Good to know
- A little extra water is fine if you accept wetter moulds and longer extraction times, but it can cause settling.
- Darvan and water amounts may need adjusting for your materials.
- Keep a batch log. Note the date, batch size, Darvan used, specific gravity, viscosity and anything you changed, so each batch starts closer to the slip you want.