High temperature, slightly sandy, plastic, semi-vitreous, grey-buff burning, general purpose, native body for reduction and
oxidation fired functional stoneware.
H550 is widely used by production potters and small companies for all types of functional and decorative stoneware. For many years
H550 has been a standard among Plainsman customers for cone 10 reduction functional ware. We maintain the porosity at about
1.5-1.8% for cone 10R, this is the lowest safe level that avoids bloating. See H450 for a smoother, lighter burning, but not quite
as vitreous material.
Process Properties
H550 is chosen for its robust combination of drying properties, green strength, and working character. It has a slightly sandy
texture and generates plenty of slip during throwing. H550 has a good distribution of particle sizes in the plus 325 mesh range
(it draws from the illite, ball clay and kaolinite mineral families) to give relatively fast drying and high green strength.
However, since H550 has a fairly high dry shrinkage, care and attention in drying are still necessary in making larger pieces,
especially flat plates and shallow bowls.
Firing
 Cone 10ox |
 Cone 10r |
H550 is the most vitreous of our high temperature buff burning materials made exclusively from our native materials. The fired
maturity of H550 has been tuned so that it offers a good compromise between vitrification and warping during firing (H450 smoother
and a little cleaner and ligher burning).
In oxidation H550 burns to a much lighter grey buff than it does in reduction. It displays some color variegation in many
reduction kilns because cone 10R is at its transition point from reduction light-buff to grey buff. The color transition radiates
from microscopic areas where fluxing begins, and as firing proceeds past cone 10 these darker grey areas invade the entire
buff-colored surface.
Since H550 contains some free silica, some care is required when heating and cooling it through quartz inversion temperatures,
especially if ware is being refired.
Glazing
Since H550 contains more than 70% SiO2 you can expect it to accept most typical cone 10 glazes without crazing them, glazes which
craze on porcelain bodies will often fit well on H550. It is still possible to get crazing with glazes high in sodium and
potassium or very low in silica or alumina. Thus you should watch out for high feldspar low flint/kaolin glazes (these are quite
common). We recommend a boiling water:ice water immersion test to make sure glazes fit well. Please contact Plainsman if you need
help to adjust your glazes.
Glaze Recipes
You can develop a compatible glossy or matte base for this body from our suggested starting point base recipes available on our
Internet web site at http://digitalfire.com/education/glaze/cone10.htm. Information is given on how to fit the glaze to your body
and how to customize it it for colors, opacity, speck, variegation, etc. For slip decoration, be careful to match drying and fired
shrinkage of the slip with the body since low temperatures generate little glass to adhere the slip.
Thermal Expansion
The chart shown was produced from a specimen fired once to cone 10 reduction in the Plainsman lab and tested in an Orton
dilatometer. If you fire to a different temperature, employ different heatup or cooldown rates, or glaze-fire more than once the
thermal expansion in your ware may be different than this chart indicates.
Average: 6.2
Physical Properties
Drying Shrinkage: 6.0-7.0%
Water Content: 20.5-21.5%
Drying Factor: C120
Dry Density: 2.0
Sieve Analysis (Tyler mesh):
+48: 0-0.3%
48-65: 1.5-2.5
65-100: 6.0-8.0
100-150: 3.0-5.0
150-200: 4.0-7.0
200-325: 7.0-9.0
Fired Shrinkage:
Cone 8: 5.7-6.7%
Cone 10: 6.0-7.0
Cone 10R: 6.0-7.0
Fired Absorption:
Cone 8: 2.5-3.5%
Cone 10: 1.5-2.5
Cone 10R: 1.5-2.5
Chemical Analysis
CaO 0.2
K2O 1.7
MgO 0.6
Na2O 0.1
TiO2 0.7
Al2O3 19.0
P2O5 0.0
SiO2 69.8
Fe2O3 1.6
MnO 0.0
LOI 6.4%
News
We continue to monitor this body closely for maturity. We want it to be as vitreous as possible but also to have a margin against
bloating. In 2006 we added H450 to our line of bodies, it is smoother and a little less vitreous that H550.
 |
Plainsman Clays Ltd.
702 Wood Street, Medicine Hat, Alberta T1A 1E9
Phone: 403-527-8535 FAX:
403-527-7508
Email: plainsman@telus.net
|
Top |